GB/T 38513-2020Methods for chemical analysis of niobium hafnium alloys - Determination of hafnium, titanium, zirconium, tungsten, tantalum contents - Inductively coupled plasma atomic emission spectrometry (English PDF)
铌铪合金化学分析方法 铪、钛、锆、钨、钽等元素的测定 电感耦合等离子体原子发射光谱法
This is a limited preview
Buy now to download the full PDF (15 pages)
Need quotation for your management?
Get a formal quotation for GB/T 38513-2020 in 30 minutes.
Issued by
SAMR; SAC
Level / Type
National · Recommended
Issue date
March 6, 2020
Implementation date
February 1, 2021
Scope
GB/T 38513-2020 is the English-translated version of 铌铪合金化学分析方法 铪、钛、锆、钨、钽等元素的测定 电感耦合等离子体原子发射光谱法.
GB/T 38513-2020 is the Chinese standard "Methods for chemical analysis of niobium hafnium alloys - Determination of hafnium, titanium, zirconium, tungsten, tantalum contents - Inductively coupled plasma atomic emission spectrometry".
Its scope clause reads: This standard specifies the determination of hafnium (Hf), titanium (Ti), zirconium (Zr), and zirconium (Zr) in niobium-hafnium alloys by inductively coupled plasma atomic emission spectrometry.
Method of tungsten (W) and tantalum (Ta) content. This standard applies to the determination of hafnium, titanium, zirconium, tungsten, and tantalum content in niobium-hafnium alloys.
The measurement range is shown in Table 1. Table 1 Measuring range of the content of each element in the niobium-hafnium alloy. Its clauses include principle; reagent; equipment; samples; test procedure; test data processing; precision; test report.
Found what you need?
Document preview — GB/T 38513-2020
National Standard of the People's Republic of China
- ICS
- 77.120.99
- Classification
- H 14
Issued by: State Administration for Market Regulation; Standardization Administration of the PRC
Contents
- 1 Scope
- 2 Principle
- 3 reagent
- 4 Equipment
- 5 samples
- 6 Test procedure
- 7 Test data processing
- 8 Precision
- 9 Test report
1 Scope
This standard specifies the determination of hafnium (Hf), titanium (Ti), zirconium (Zr), and zirconium (Zr) in niobium-hafnium alloys by inductively coupled plasma atomic emission spectrometry.
Method of tungsten (W) and tantalum (Ta) content.
This standard applies to the determination of hafnium, titanium, zirconium, tungsten, and tantalum content in niobium-hafnium alloys. The measurement range is shown in Table 1.
Table 1 Measuring range of the content of each element in the niobium-hafnium alloy
2 Principle
The sample is dissolved with hydrofluoric acid and nitric acid, and an inductively coupled plasma atomic emission spectrometer is used to measure the test at the recommended analysis line wavelength.
The emission intensity of each element in the liquid, the mass concentration of each element is obtained from the working curve, and the content of each element is calculated.
3 reagent
Unless otherwise specified, only reagents and laboratory secondary water confirmed to be pure superior grade are used in the analysis.
3.1
Nitric acid (rho=1.42g/mL).
3.2
Hydrofluoric acid (rho=1.13g/mL).
3.3
Hydrochloric acid (rho=1.19g/mL).
3.4
Niobium metal (wNb>=99.95%).
3.5 Titanium standard solution
accurately weigh 0.1000g of metallic titanium (wTi>=99.99%) into a 100mL polytetrafluoroethylene beaker and add
10mL water, 5mL hydrochloric acid (3.3), 2mL hydrofluoric acid (3.2), 1mL nitric acid (3.1), dissolve, cool, transfer into a 100mL plastic volumetric flask
Dilute to the mark with water and mix well. 1mL of this solution contains 1mg of titanium.
3.6 Zirconium standard solution
Weigh 0.1000g of metallic zirconium (wZr>=99.99%) into a 100mL PTFE beaker, add 10mL of water,
2mL hydrofluoric acid (3.2), 1mL nitric acid (3.1), dissolve, cool, transfer into a 100mL plastic volumetric flask, dilute to the mark with water, and mix.
This solution 1mL contains 1mg zirconium.
3.7 Tungsten standard solution
Weigh 0.1000g metallic tungsten (wW>=99.95%) into a 100mL PTFE beaker, add 10mL nitrate
Acid (3.1), 3mL hydrofluoric acid (3.2), dissolve, cool, transfer to a 100mL plastic volumetric flask, dilute to the mark with water, and mix. This solution
1mL contains 1mg tungsten.
3.8 Tantalum standard solution
Weigh 0.1000g metallic tantalum (wTa>=99.99%) into a 100mL polytetrafluoroethylene beaker, add 5mL nitric acid (3.1), add 5 mL of hydrofluoric acid (3.2) in portions, cover with a PTFE watch glass, heat to dissolve at low temperature, cool, and transfer to a 100 mL plastic container
In a measuring flask, dilute to the mark with water and mix well. 1mL of this solution contains 1mg of tantalum.
3.9 Hafnium standard solution
Weigh 0.1000g metal hafnium (wHf>=99.99%) into a 100mL PTFE beaker, add 10mL water,
2mL of hydrofluoric acid (3.2), dissolve, cool, transfer to a 100mL plastic volumetric flask, dilute to the mark with water, and mix. This solution 1mL contains
1mg hafnium.
4 Equipment
4.1 Inductively coupled plasma atomic emission spectrometer
with hydrofluoric acid resistant sampling system, resolution less than 0.006nm (200nm).
4.2
The recommended analysis line wavelength of each element is shown in Table 2.
Table 2 Recommended analysis line wavelength of each element
5 samples
Process the sample into chips with a length not greater than 5mm.
6 Test procedure
6.1 Sample
Weigh 0.20g sample (Chapter 5), accurate to 0.0001g.
6.2 Parallel test
Do two tests in parallel and take the average value.
6.3 Blank test
Weigh the metal niobium (3.4) of the same quality as the sample, and do a blank test with the sample.
6.4 Preparation of analysis test solution
6.4.1
Preparation of analysis test solution A
Place the sample (6.1) in a 150mL polytetrafluoroethylene beaker, add 10mL water, 2mL hydrofluoric acid (3.2), 5mL nitric acid (3.1),
Heat in a water bath, wait for the sample to dissolve completely, cool it, transfer it to a 100mL plastic volumetric flask, dilute to the mark with water, and shake well.
6.5 Preparation of working curve solution
6.5.1
Preparation of working curve standard solution A
Weigh 0.20g of metallic niobium (3.4) into a set of 150mL PTFE beakers, and dissolve them according to step 6.4.1.After cooling
Transfer to a set of 100mL plastic volumetric flasks, add standard solutions of titanium, zirconium, tungsten, and tantalum according to Table 3, dilute to the mark with water, and shake well.
Table 3 The addition amount of each element standard solution in the working curve
6.5.2 Preparation of working curve standard solution B
Weigh 0.20g of metallic niobium (3.4) into a 150mL PTFE beaker, dissolve it according to step 6.4.1, and transfer it after cooling.
In a 100mL plastic volumetric flask, dilute with water to the mark. After mixing, pipette 10.00mL into a set of plastic volumetric flasks, and add hafnium according to Table 3.
Standard solution, respectively add 2mL hydrofluoric acid (3.2), dilute to the mark with water, shake.
6.6 Determination
Introduce the working curve solution into the inductively coupled plasma atomic emission spectrometer. According to the best measurement conditions of the instrument selected for the experiment, select
At the specified wavelength, determine the emission intensity of each element in the series of working curve solutions. When the linear correlation coefficient of the working curve is >=0.999, it can be
Analyze the measurement of the test solution, and the computer automatically gives the mass concentration of each element according to the relationship between light intensity and concentration.
7 Test data processing
The content of each element is calculated as the mass fraction wx and calculated according to formula (1).
8 Precision
8.1 Repeatability
The measured values of two independent test results obtained under repeatability conditions are within the range of the average value given in Table 4.
The absolute difference does not exceed the repeatability limit (r), and the case of exceeding the repeatability limit (r) does not exceed 5%. Repeatability limit (r) is linear according to the data in Table 4
Obtained by interpolation or extension.
Table 4 Repeatability limits
8.2 Reproducibility
The measured values of two independent test results obtained under reproducibility conditions are within the range of the average value given in Table 5.
The absolute difference does not exceed the reproducibility limit (R), and the case of exceeding the reproducibility limit (R) does not exceed 5%. Reproducibility limit (R) adopts the line according to the data in Table 5
Obtained by sexual interpolation or extension method.
Table 5 Reproducibility limits
9 Test report
The test report should give at least the following aspects.
---Test object;
---This standard number (note the date);
--- Anomalies observed;
---Test date.
......
This preview omits tables, figures, formulas and parts of the technical clauses. The complete document — 15 pages — is available in the English PDF.
Similar standards
How to Download GB/T 38513-2020
- 1
Add to cart
Click "Download PDF" on this page and choose "Buy this standard". You can add more standards before checkout.
- 2
Checkout
Enter your email and billing details. Payment is processed securely by Stripe (cards or bank transfer). Prefer bank details? Request a quotation (min. order $300).
- 3
Fast delivery
After payment you'll receive an email confirmation. The English PDF is sent to the same address, usually within minutes and at the latest within 1 business day.
- 4
Invoice included
A tax invoice is attached to the confirmation email. Need a custom invoice? Contact us.
Related Standards
GB/T 10003-2026 — Biaxially oriented polypropylene (BOPP) film
GB/T 10004-2026 — Plastic/Plastic laminated films and pouches for packaging
GB/T 10007-2026 — Rigid cellular plastics - Determination of shear properties
GB/T 38513-2020
$145.00