GB/T 38684-2020Metallic materials - Sheet and strip - Biaxial stress-strain curve by means of bulge test - Optical measuring systems (English PDF)
金属材料 薄板和薄带 双轴应力-应变曲线胀形试验 光学测量方法.
This is a limited preview
Buy now to download the full PDF (30 pages)
Need quotation for your management?
Get a formal quotation for GB/T 38684-2020 in 30 minutes.
Issued by
SAMR; SAC
Level / Type
National · Recommended
Issue date
March 31, 2020
Implementation date
October 1, 2020
Scope
GB/T 38684-2020 is the English-translated version of 金属材料 薄板和薄带 双轴应力-应变曲线胀形试验 光学测量方法..
GB/T 38684-2020 specifies the symbols and descriptions, the principle, the test equipment, the optical measurement system, the specimen, the test procedure and the evaluation method for apex curvature deformation and strain of the optical measuring method used in the bulge test for the biaxial stress-strain curve of metallic sheet and strip, together with the calculation of the curve and the test report.
It fixes what the equipment must do: the system determines the XYZ coordinates of the grid points on the surface of the bulged specimen without contact and from them the true strains and the radius of curvature of the dome; the concave die, the blank holder and the fluid cavity must be rigid enough, the pressurizing fluid must be in full contact with the specimen, and a glass plate is recommended in front of the lens against oil splash at rupture.
The optical system should use two or more cameras, and no more than 5 % of the measurement points may be lost.
A normative annex gives the verification procedures for the optical measurement system, and two informative annexes the curvature calculation based on a response surface and the determination of the equibiaxial stress points of the yield and work hardening curves.
It applies to the determination of the biaxial stress-strain curve of metallic sheet and strip less than 3 mm thick during pure bulging. It is a modified adoption of ISO 16808:2014, was issued on 31 March 2020 and has applied since 1 October 2020.
Found what you need?
Document preview — GB/T 38684-2020
National Standard of the People's Republic of China
- ICS
- 77.040.10
- Classification
- H 22
Issued by: SAMR; SAC
Contents
- Foreword3
- 1 Scope5
- 2 Symbols and descriptions5
- 3 Principle6
- 4 Test equipment7
- 5 Optical measurement system10
- 6 Specimen10
- 7 Test procedure11
- 8 Evaluation method of apex curvature deformation and strain12
- 9 Calculation of biaxial stress-strain curve14
- 10 Test report15
- Appendix A (Normative) Verification procedures for optical measurement systems17
- Appendix B (Informative) Curvature calculation based on response surface20
- Appendix C (Informative) Determination of equiaxial stress points of yield and work hardening curves22
- References30
1 Scope
This standard specifies the symbols and descriptions, principles, test equipment, optical measurement systems, specimens, test procedures, apex curvature deformation and strain evaluation method for the optical measurement method for the biaxial stress-strain curve bulging test of sheets and strips of metallic materials, as well as the calculation and test report of biaxial stress-strain curve.
This standard applies to the determination of biaxial stress-strain curve of the metallic sheet and strip which has a thickness of less than 3 mm during the pure bulging process.
Note: The term "biaxial stress-strain curve" in this standard is abbreviated. The test determines the "biaxial true stress-true strain curve".
2 Symbols and descriptions
The symbols and descriptions used in this standard are as shown in Table 1.
4 Test equipment
4.3 During the test, the system shall be able to determine the XYZ coordinates (non-contact) of the grid points on the surface of the bulged specimen through the optical system; use these coordinates to calculate the true strain epsilon1 and epsilon2 of each grid point in the selected area, the thickness direction strain epsilon3, as well as the curvature radius rho of the dome of the bulging specimen.
4.4 The system should be equipped with a fluid pressure measurement system or an indirect measurement system. Starting from 20% of the maximum range of the system, the accuracy of the measurement system should meet level 1 requirements.
4.5 The concave die, blank holder and liquid cavity shall have sufficient rigidity, to ensure the minimum deformation of these parts during the test. The blank holding force shall be high enough to ensure the tightness of the blank holder. The specimen shall not move between the blank holder and the concave die. Usually during the test, the bulging pressure will weaken the blank holding force. When determining the blank holding force required for the test, it shall consider the effect of this effect on the blank holding force.
4.6 The fluid medium for pressurization shall be in full contact with the surface of the specimen (no bubbles), to prevent the occurrence of high energy pressure release or oil splash due to the energy storage effect of the compressed air bubbles at the moment of energy release or rupture. During the test, until the specimen ruptures, the fluid shall not leak through the blank holder, concave die, or plate and anywhere else.
4.7 It is recommended to use calendering ribs (or devices with similar shapes on a round surface) to prevent material flow. The use of calendering ribs shall not cause the material to crack. The position of the calendering rib can be located between the concave die and the blank holder. The size of the calendering ribs should avoid blocking the material from flowing during the test, thereby causing excessive bending and wrinkling of the material.
4.8 It is recommended to place a glass plate in front of the lens and lighting equipment, to ensure that when the specimen is broken, the splash of test oil will not affect the optical measurement system. The glass plate can be fixed on the blank holder (thick glass) or placed in front of the lens and lighting system (thin glass), as shown in Figure 3. This plug-in protection device shall not affect the measurement quality of the optical measurement system. After each test, the glass plate shall be wiped clean to avoid damage or scratches; Meanwhile it shall be accurately placed back to the original position so that no recalibration of the measurement system is required. In order to obtain better measurement
5 Optical measurement system
In order to determine the radius of curvature rho of the specimen surface, as well as the true strains epsilon1 and epsilon2, it is recommended that the optical measurement system have the following characteristics:
a) Optical sensors based on 2 or more cameras.
b) The measurement range shall be greater than 1/2 of the concave die's diameter. The measurement area used should be a concentric circle of the blank holder; its diameter shall be greater than half the diameter of the blank holder. Throughout the forming process, this area can be observed at any height of the drawn specimen.
c) Local resolution (distance between two individual grid points): The distance gmax between two adjacent measurement points on the undeformed specimens shall meet the following requirements:
d) The determination of the curvature requires that in the concentric circle area of the blank holder with a diameter of 1/2 ddie, the measurement accuracy can be verified by testing the optical measurement system, as shown in Appendix A. The accuracy of the z-axis coordinate shall meet:
Note: Strain measurement accuracy: rms (epsilon1) = 0.003, rms (epsilon2) = 0.003.
For each of the true strain values as mentioned in the root mean square above, the acceptable measurement range is as follows:
- epsilonreal = 0, acceptable measurement range: -0.003 ~ 0.003;
- epsilonreal = 0.5, acceptable measurement range: 0.479 ~ 0.503.
e) Lost measurement points: In order to avoid curvature discontinuities, in concentric circles with a diameter half the diameter of the blank holder, only measurement points that do not exceed 5% (not including interpolated points) are allowed to be lost. If two adjacent points are lost, the point shall not be fitted into the circle.
6 Specimen
6.1 General
7 Test procedure
7.2 Measure the initial thickness of the specimen, accurate to 0.01 mm.
7.3 Press the specimen through the blank holder and concave die. During the test, air bubbles shall be avoided between the specimen and the hydraulic fluid medium, to prevent the compressed air from splashing the hydraulic oil when the specimen ruptures.
7.4 It is recommended to use a constant strain rate of 0.05 s-1 for the deformation area of the specimen. If a constant strain rate cannot be achieved, it should keep the constant speed of the punch or hydraulic fluid medium. In the process of measuring the biaxial stress-strain curve, in order to avoid a greater impact on materials that are sensitive to temperature or strain rate, the bulge test should be completed within 2 min ~ 4 min.
7.5 During the test, measure the pressure of the hydraulic fluid medium.
7.6 During the test, measure the XYZ coordinates of the grid points on the specimen surface. Among them, the origin of coordinates shall be located at the center of the blank holder. The XY plane is parallel to the surface of the blank holder (parallel to the metal plate pressed before the test). Moreover, the X-axis direction corresponds to the rolling direction. The Z-axis shall be perpendicular to the surface of the clamped metal sheet specimen and face the direction of the optical sensor.
7.7 Pressure data and forming data shall be measured and saved simultaneously. It is recommended to measure at least 100 sets of data during the test. In order to show the entire strain and pressure changes, it is recommended to record at least 100 pictures of the bulge test.
7.8 When the crack completely penetrates the thickness direction of the specimen, the specimen shall be considered to have failed. That is, cracks in the thickness direction of the specimen can be judged by detecting the drop in fluid pressure.
7.9 Prepare enough specimens, to ensure that at least three valid test results are obtained.
8 Evaluation method of apex curvature deformation and strain
8.1 In order to better explain the following calculation methods of curvature and strain, it is necessary to assume a spherical surface (best fit spherical surface) near the apex. In a picture before the failure of the specimen, as defined in 7.8, select the arc top area with the largest deformation; define it as the location where the true stress and true thickness strain epsilon3. In order to obtain a stable
9 Calculation of biaxial stress-strain curve
9.3 The ratio of the diameter of the concave die and the thickness of the specimen shall be larger within a reasonable range, so as to ensure that the specimen is under a thin-walled stress state, meanwhile it may ignore the influence of bending. For tests where the ratio of the concave die's diameter to the specimen thickness is less than 100, it is recommended to check whether the bending strain is sufficiently small compared to the actual thickness strain epsilon3. The formula for determining the bending strain is as shown in formula (9):
Note: The biaxial stress-strain curve was obtained without using any assumptions based on the yield criterion. The biaxial stress-strain curve can be used to determine the yield locus of equiaxed stress, and to estimate the work hardening curve of the material before it reaches uniform extension.
9.4 Appendix C gives the recommended method for obtaining the yield criterion of equal biaxial stress points and the method for extrapolating the equivalent stress-strain curve based on uniaxial tensile specimens from the biaxial stress-strain curve obtained by hydraulic bulge test.
10 Test report
The test report shall contain at least the following information:
a) Number of this standard;
b) Operator;
c) Material designation;
d) The initial thickness of specimen;
e) Grid, camera and software used;
f) Location of protective glass;
g) Tonnage of test equipment;
h) Bulging or piston speed;
i) The calculation method of bulge test, especially the parameters for calculating curvature and average strain;
j) The number of repeated tests;
k) For each bulge test, a table is required to record the absolute values of […]
Appendix C (Informative) Determination of equiaxial stress points of yield and work hardening curves
C.1 Overview
In the hydraulic bulge test to obtain an equal biaxial stress-strain curve, the average value of the primary stress and secondary stress corresponds to the absolute value of the plastic true thickness strain. Generally, the true stress-strain curve obtained from the uniaxial tensile test in the rolling direction can be used as a reference curve for calculating the material hardening and yield point.
By comparing the stress-strain data of the iso-biaxial stress state and the uniaxial reference curve, it can calculate the iso-biaxial stress point, meanwhile the iso-biaxial strain curve can be transformed into an equivalent stress-strain curve, which provides the work hardening data when the strain is higher than the uniform strain of tensile test. C.2 describes how to determine the equal biaxial stress ratio and how to extend the results of the bulge test on the uniaxial stress-strain curve to more than uniform elongation.
C.2 Procedure
C.2.1 The procedure described below is one of the methods to deal with stress-strain data in the bulge test. It is the user's responsibility to check whether the basic assumptions are fully satisfied before using this method, so that this method is consistent with the actual material behavior. If in doubt, it is strongly recommended to consult experts in this field. The assumptions made by this procedure are as follows:
- Isotropic hardening;
- The yield locus shape does not change with strain;
- Work hardening has nothing to do with the strain path (stress path);
- The loading path and strain path of the test are constant;
- The strain rate and temperature of the bulge test are close to those of the tensile test. If this condition is not met, the effect of strain rate and temperature on the material strength shall be known, to determine whether correction is required.
C.2.2 The true strain epsilon1-UE of uniform elongation as obtained by the tensile test in the rolling direction is taken as the reference point of the equivalent strain epsilonE- […]
......
This preview omits tables, figures, formulas and parts of the technical clauses. The complete document — 30 pages — is available in the English PDF.
How to Download GB/T 38684-2020
- 1
Add to cart
Click "Download PDF" on this page and choose "Buy this standard". You can add more standards before checkout.
- 2
Checkout
Enter your email and billing details. Payment is processed securely by Stripe (cards or bank transfer). Prefer bank details? Request a quotation (min. order $300).
- 3
Fast delivery
After payment you'll receive an email confirmation. The English PDF is sent to the same address, usually within minutes and at the latest within 1 business day.
- 4
Invoice included
A tax invoice is attached to the confirmation email. Need a custom invoice? Contact us.
Related Standards
GB/T 10003-2026 — Biaxially oriented polypropylene (BOPP) film
GB/T 10004-2026 — Plastic/Plastic laminated films and pouches for packaging
GB/T 10007-2026 — Rigid cellular plastics - Determination of shear properties
GB/T 38684-2020
$235.00